The density of both wrought and cast Zeron 100 is 7840 kg/m3 or 489 lb/ft3 (7.84g/cm3 ) at 68°F (20°C).
Typical specific heats for both wrought and cast Zeron 100.
Temp,°F (°C) |
Specific Heat, |
J Kg-1 K-1 |
Btu/lb °F |
68 (20) |
482 |
0.115 |
212 (100) |
500 |
0.119 |
302 (150) |
513 |
0.122 |
392 (200) |
523 |
0.125 |
482 (250) |
535 |
0.128 |
572 (300) |
547 |
0.13 |
Typical values for wrought Zeron 100.
Linear Thermal Expansion Coefficient, 10-6 K-1 |
Temp, °C |
20 - 100 |
20 - 200 |
20 - 300 |
Zeron 100 |
12.8 |
13.3 |
13.8 |
Carbon Steel |
11.5 |
12.2 |
12.9 |
Austenitic Stainless Steel |
16.8 |
17.2 |
17.6 |
Linear Thermal Expansion Coefficient, 10-6 in/in °F |
Temp, °F |
70 - 200 |
70 - 400 |
70 - 600 |
Zeron 100 |
7.1 |
7.4 |
7.7 |
Carbon Steel |
6.4 |
6.8 |
7.2 |
Austenitic Stainless Steel |
9.3 |
9.6 |
9.8 |
Typical values of resistivity are shown below
At room temperature the peak relative magnetic permeability of Zeron 100 is typically 29.
The modulus is a function of austenite/ferrite ratio and production route. Variations of + 5% are found with both wrought and cast products. The typical value for Zeron 100 at room temperature is 29,000 ksi (200 GPa). The Young’s Modulus decreases slightly with increasing temperature as shown below.
The typical value for Zeron 100 at room temperature is 0.32
Surface Treatments
- Xylan 1070 / 1014 / 1400 / 1424
- Xylar 2 / 101
- SermaGard 1105 / 1280
- Dacromet 320 / 500
- TakeCoat 1000 Ceramic
- Magnigard
- MolyKote
Certifications
- ISO 9001 - 2015 Certified
- PED 2014/68/EC
- NACE MR0175/ISO 15156-2
- NORSOK M-650 MDS 055
- DFAR
- MERKBLATT AD 2000 W2/W7/W10